Posted (edited)

It took about 16 hrs to clean most of the scale off. I may have to do some tumbeling in conjunction with an. etch

Edited by Jan Ysselstein
Posted (edited)

AchimIMG_0028.jpeg Wirtz once suggested makers in history used a lot of debris associated with iron making and processing. At the time I thought that not to be the case. Fast forward about 10 years……I have always saved that debris and now I have a vibratory tumbler……suddenly Achim was making sense…of course. The material shown below was pulled with a magnet from the charcoal in the furnace….I never pulled a hot bloom unless it was a demo. I would approach a sealed fufnace the next day, extract 100% of what was there …some of it was this debris. Now I think it is precious as a possible ingredient …high in carbon and 100% from the magnetic ore. Here are some pics .

IMG_0030.jpeg

IMG_0028.jpeg

Edited by Jan Ysselstein
  • Like 3
Posted (edited)

Here is the cleaning process…a constant flow of black dust rising . The next melt will include 2/3 of this material and some  very low carbon bloom. If I can tune it in it should last for a while.

Edited by Jan Ysselstein
  • Like 1
Posted

They certainly look like little metal nuggets. These were the leftovers from the furnace smelt?

“So I'm lightin' out for the territory, ahead of the scared and the weak and the mean spirited, because Aunt Sally is fixin’ to adopt me and civilize me, and I can't stand it. I've been there before.”

The only bad experience is the one from which you learn nothing.  

 

Josh

http://www.dosgatosdesignsllc.com/#!

https://www.youtube.com/channel/UCdJMFMqnbLYqv965xd64vYg

J.States Bladesmith | Facebook

https://www.facebook.com/dos.gatos.71

https://www.etsy.com/shop/JStatesBladesmith

Posted

Those are little prills of cast iron that didn't consolidate into the main mass.  Low carbon blooms do that as well, but don't make such nice little nuggets.

  • Like 1
Posted

Yes, those are sorted by size. I have bigger ones…the very small ones I just call ore. I will start by arbitrarily assigning the above bits a 2.8 % C content. We will see what that produces and adjust our thinking based on that. There is about 65 lbs of that material on the shelf so using it would be a big bonus.

  • Like 1
  • 2 months later...
Posted (edited)

So, things don’t always go as they should. Below is a pic of some failed recent runs, which I hope to rerun next. All are chemically 100% steel from ore. Should have one by tonight. The total weight is 9500 grams.

IMG_1210.jpeg

Edited by Jan Ysselstein
  • Like 2
Posted (edited)

Never a dull moment so many distractions. I have just completed two runs 1 made another discard (rework) the other is too fresh for me to figure it out. Todays ingot looks good , has a shrink cavity nicely located…..I am very happy with the results. Also located an old ingot from the scrap pile with similar patterning on the top surface. The patterning looks very much like some of the ingots from “ hoard” which I will link in a day or so. 
A couple of the rework ingots in the above picture were broken on the press and to my surprise look and spark very much like Japanese Jewel steel. They will be used to make some knives by folding. Here are some pics. The bottom picture is of an older discarded ingot. 1828 grams is today’s ingot.

The older ingot was culled because it has too high a carbon level.

 

IMG_1225.jpeg

Today’s ingot

IMG_1226.jpeg
Today’s ingot

IMG_1227.jpeg
broken rework

IMG_1230.jpeg
broken rework

IMG_1232.jpeg
older ingot same pattern on surface

IMG_1238.jpeg
Today’s ingot side view.

Edited by Jan Ysselstein
  • Like 2
  • 2 weeks later...
Posted (edited)

I took the older high carbon cast iron ingot ….guessed the carbon content , added some low carbon iron and created a new ingot…..the spark looks ok. The top of the resulting ingot is a little rough ….probably due to air entering the top of the crucible. Here are a couple of pics. We have exchanged the cold top for a shrinkage cavity . I will take these two ingots to 1150 C for 4 hrs and quench them to room temperature, cut them in two and forge.

The ingot weighs 1990 grams.

IMG_1474.jpegSide view of remelted ingot

IMG_1469.jpegTop view of remelted ingot

IMG_1470.jpeg

Edited by Jan Ysselstein
Posted (edited)

Both ingots have soaked for 3.5 hrs at 1150 C. They were quenched in moving air , the kiln wash was removed. Included in the furnace were 3 old culled half ingots.  Now I , cut in half and will look at the grain and gently begin forging. One of the large ingots has a rough center….all I want to see should forge out. Here are some pics .

IMG_1703.jpeg

IMG_1702.jpeg

IMG_1704.jpeg

Edited by Jan Ysselstein
  • Like 1
Posted (edited)

The ingots were cut and I looked at their granular structures. Everything looked as expected but some areas  in one of the ingots may still have some primary cementite in place (very little ). If I can figure out how to post them from the photo software I will post them. Here are a couple of cross section macros. The rough center ingot is pretty obvious.

IMG_1482.jpeg

IMG_1480.jpeg

Edited by Jan Ysselstein
  • Like 1
  • 2 weeks later...
Posted

Top photo shows the micro structure of the ingot with the rough top .

The bottom two show the structure of the other ingot. Both ingots were held at 1150 C for 3.5 hrs.

I hope to forge them in a day or two.

Photo on 4-30-25 at 7.17 PM.jpg

Photo on 4-30-25 at 7.11 PM.jpg

Photo on 5-1-25 at 8.55 PM.jpg

  • Like 2
Posted

Those look really good Jan.

On 5/11/2025 at 11:25 PM, Jan Ysselstein said:

Both ingots were held at 1150 C for 3.5 hrs.

Note to self.....

  • Thanks 1

“So I'm lightin' out for the territory, ahead of the scared and the weak and the mean spirited, because Aunt Sally is fixin’ to adopt me and civilize me, and I can't stand it. I've been there before.”

The only bad experience is the one from which you learn nothing.  

 

Josh

http://www.dosgatosdesignsllc.com/#!

https://www.youtube.com/channel/UCdJMFMqnbLYqv965xd64vYg

J.States Bladesmith | Facebook

https://www.facebook.com/dos.gatos.71

https://www.etsy.com/shop/JStatesBladesmith

Posted

It could have gone better , but I have the info I need to move on. So far the rough top is looking pretty good …..I have a good supply for making small knives should I want to do that. 
The shrinkage cavities did create problems …..I will give up on that approach if I cannot deal with that material on the next run. Next run is to repeat ( as close as possible) the open crucible rough top melt. This time I will make sure the top is closed 

I have a few poor photos of the rough top ingot after about 5 heats and the carbon is still everywhere…I will thermal cycle it and post some pics if it is dramatic.

  • Like 1
Posted

After about 5 forging cycles I did not find any large cementite …all forging was done with the press . Pattern is evident at 5 forging cycles. I have a press forging problem which I can easily fix. To avoid using direct line of sight I run slightly off center dies and let the movement of the metal tell me when to change direction…..this creates a large bend and eventually leads to cracking.

  • Like 1
Posted

Below are a couple of pics of the smaller grain size ingot. Very few severe press forging cycles. There does seem to be a pattern ( at least a contrast ) .Looking for an area ratio of light and dark ( what is light now will etch dark later) . Also looking for clean edges from light to dark. I will try to avoid the forging mistakes. Somewhere in the pile are the parts for a hammer specifically designed for forging “wootz. I will thermal cycle the two bars and update.

 

Photo on 5-16-25 at 12.49 PM #2.jpg

Photo on 5-16-25 at 12.44 PM.jpg

  • Like 3
  • 1 year later...
Posted (edited)

OK the above bar will have to wait until I find it again….it is one of many. I would like to get into this thread again….test a few ideas and exit this Winter.

Right now an exit looks like a lens bottomed crucible fired over charcoal to completion.

 

Now  off to build an 8” diameter crucible furnace..

 

The next series of ingots will be targeting a specific volume ,for example say one would like to process an ingot large enough to make several knives or a sword……we would need enough steel to make a bar 3/16” x 2” x36” or 13.5 cubic inches of ingot….that ingot will have to weigh at least 1850 grams.  I will start at 1500 grams and work my way up.

Edited by Jan Ysselstein
Posted (edited)

The crucible is holding about 1450 grams. E- iron, cast iron , charcoal. Hoping to find out if my cast iron is high enough in carbide formers and will produce a pattern at 600 grams out of  1450 grams total.

I will fire the crucible Wednesday if all goes well.

Edited by Jan Ysselstein
  • Like 1
Posted

The crucible is approaching historic shapes…..the top will soon be modified to allow handling with tongs.

Posted (edited)
On 8/25/2026 at 9:00 PM, Jan Ysselstein said:historic shapes…..the top will soon be modified to allow handling with tongs.

 

On 8/25/2026 at 9:00 PM, Jan Ysselstein said:handling with tongs.

I finally got a chance to fire the furnace with the new crucible. So far so good I am about to allow it all to cool and will share the results regardless their appearance.

IMG_5075.jpeg

IMG_5074.jpeg

IMG_5072.jpeg

Edited by Jan Ysselstein
  • Like 2
Posted (edited)

 No slag was added to this melt….I ran the furnace in a reduction mode most of the run. That approach may have cost me some heat , resulting in unincorporated e iron. All in all …I am very happy with the results. The ingot weight is exactly what went into the crucible ….wow. I have one more this size and several an inch smaller …onward we go.I will cut this in half and have a look inside….it should all be pearlite. The unincorporated e iron has picked up a lot of carbon as seen  by the spark test.V

The ingot is 4.5” diameter, 1” thick at its thickest place.

 

IMG_5114.jpeg

IMG_5113.jpeg

IMG_5112.jpeg

IMG_5106.jpeg

 

Edited by Jan Ysselstein
  • Like 2
Posted (edited)

A slight change in the plan. I will do a little grinding around the edges to allow the ingot to fit into another crucible without breaking it upon heating it. We will melt again at 1/2 hrs. heating and 1/2 hours homogenizing at max temp.

So, we have learned a lot in a day, most importantly is the furnace appearance when the fuel/air mixture is too rich….very useful, slag may not be needed, 

 

 

 

IMG_5036.jpeg

 

 

 

 

 

 

 

 

 

 

IMG_5124.jpeg

IMG_5121.jpeg

 

Edited by Jan Ysselstein
  • Like 1
Posted (edited)

Good news/ bad news …..very pleased..

As soon as I figure out how to post my phone magnified pictures I will post some..

Still having some unincorporated material on the bottom side of the ingot…I am starting to think this is related to the particular shrinkage phenomenon. This may not be a big problem as I can work around it.

 

Furnace is ruined , oh well. It got very, very hot.

The top of the ingot is phenomenal ,very large dendrites. IMG_5135.jpegIMG_5139.jpeg

 

I added 200 grams of new material to the melt 50/50 cast/ e iron.  The 200 grams showed up at the end of the melt.

 

The spark test is beautiful…very much like a file.

 

I am going to work with the ingot. To find out what the bottom phenomenon might be.

As far as the historical process …..I am content with the ingot dimensions for the long run. We will get through these tech hurdles …now thoughts are about ingot melting over charcoal and the chemistry of those ingots. .

 

 

 

 

 

 

 

IMG_5133.jpeg

IMG_5126.jpeg

IMG_5125.jpeg

IMG_5137.jpeg

IMG_5136.jpeg

IMG_5125.jpeg

Edited by Jan Ysselstein
  • Like 2

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
×
×
  • Create New...